ArticleName |
Phase formation during the sintering of a Ti – Al – SiC composite material |
ArticleAuthorData |
Institute of Materials Science, Khabarovsk Research Center, Far Eastern Branch of RAS, Khabarovsk, Russia:
I. A. Astapov, Senior Researcher, e-mail: immaterial_khv@mail.ru N. M. Vlasova, Researcher T. B. Ershova, Head of Laboratory of Composite Materials E. A. Kirichenko, Researcher |
Abstract |
Currently, the development of new composite materials is an urgent task. The combination of properties in multiphase material provides advantages that can be used in aircraft and machine building, including the development of functional coatings and powders. Of these materials it is possible to distinguish composites based on MAX-phases, which are characterized by increased characteristics of heat resistance, elasticity, ease of machining, etc. Materials of composition (3Ti:Al) + 15% SiC were obtained by cold pressing and subsequent hightemperature sintering in vacuum. As initial components, chemically pure titanium, aluminum and silicon carbide were used. Thermal analysis was carried out, and phase composition and microstructure were studied. It is shown that the formation of the target phases — Ti2AlC and titanium carbosilicide — occurs in several stages and proceeds relatively slowly. On the DTA curve, only one characteristic exothermic peak corresponding to the synthesis of titanium aluminide can be observed. Phase analysis showed that at low temperatures (up to 1000 оС), an intermetallic compound of titanium with aluminum is formed. At the same time, the silicon carbide lattice is restructured with the concomitant formation of TiC and at a temperature above 1100 оС — by the formation of Ti5Si3Cx. The MAX phase of Ti2AlC is the result of the interaction of Ti3Al with the carbon atoms released during the reaction of silicon carbide with titanium. The microstructure investigation indicates the final stage of sintering at temperatures above 1300 oC. At lower values in the structure, individual grains of TiC, SiC, and Ti3Al intermetallide regions are noticeable. The sample, sintered at T = 1400 оС, is a two-phase composite material, in each grain of which Ti2AlC and Ti5Si3Cx are evenly distributed. There were no other phases in these samples. The microhardness of two-phase grains is HV50 = 7.2 GPa, while the hardness numbers are in the range 3.0–9.0 GPa, which is explained by the influence of the ratio of the two phases at the place of indentation. |
References |
1. Hu Ch., Zhang H., Li F., Huang Q., Bao Y. New phases’ discovery in MAX family. International Journal of Refractory Metals and Hard Materials. 2013. No. 36. pp. 300–312. 2. Smetkin A. A., Mayorova Yu. K. Properties of materials based on MAX-phases (a review). Vestnik PNIPU. 2015. Vol. 17, No. 4. pp. 120–138. 3. Sun Z. M. Progress in research and development on MAX-phases: a family of layered ternary compounds. International Materials Reviews. 2011. Vol. 56, Iss. 3. pp. 143–166. 4. Haftani M., Heydari M. S., Baharvandi H. R., Ehsani N. Studying the oxidation of Ti2AlC MAX phase in atmosphere : A review. International Journal of Refractory Metals and Hard Materials. 2016. Vol. 61. pp. 51–60. 5. Cao J., Yin Z., Li H., Gao G., Zhang X. Tribological and mechanical properties of Ti2AlC coating at room temperature and 800 оC. Ceramics International. 2018. Vol. 44, Iss. 1. pp. 1046–1051. 6. Nelson M., Agne M. T., Anasori B., Yang J., Barsoum M. W. Synthesis and Characterization of the Mechanical Properties of Ti3SiC2/Mg and Cr2AlC/Mg Alloy Composites. Materials Science and Engineering: A. 2017. Vol. 705. pp. 182–188. 7. Wang W., Li Q., Ma R. et al. Superior bending and impact properties of SiC matrix composites infiltrated with an aluminium alloy. Ceramics International. 2017. Vol. 43, Iss. 5. pp. 4551–4556. 8. Advances in Science and Technology of Mn+ 1AXn Phases. Ed.: I. M. Low. Woodhead Publishing (Elsevier). 2012. 474 p. 9. Fakih H., Jacques S., Dezellus O. et al. Phase Equilibria and Reactive Chemical Vapor Deposition (RCVD) of Ti3SiC2. Journal of Phase Equilibria and Diffusion. 2008. Vol. 29, Iss. 3. pp. 239–246. 10. Tang C., Klimenkov M., Jaentsch U. et al. Synthesis and characterization of Ti2AlC coatings by magnetron sputtering from three elemental targets and ex-situ annealing. Surface and Coatings Technology. 2017. Vol. 309. pp. 445–455. 11. Gorshkov V. A., Miloserdov P. A., Luginina M. A., Sachkova N. V., Belikova A. F. High-temperature synthesis of a cast material with a maximum content of the max phase Cr2AlC. Inorganic Materials. 2017. Vol. 53, Iss. 3. pp. 271–277. 12. Yan M., Chen Y., Mei B., Zhu J. Synthesis of high-purity Ti2AlN ceramic by hot pressing. Transactions of Nonferrous Metals Society of China. 2008. Vol. 18, Iss. 1. pp. 82–85. 13. Atazadeh N., Heydari M. S., Baharvandi H. R., Ehsani N. Reviewing the effects of different additives on the synthesis of the Ti3SiC2 MAX phase by mechanical alloying technique. International Journal of Refractory Metals and Hard Materials. 2016. Vol. 61. pp. 67–78. 14. Sun Z., Li M., Hu L. et al. Surface Chemistry, Dispersion Behavior, and Slip Casting of Ti3AlC2 Suspensions. Journal of the American Ceramic Society. 2009. Vol. 92, Iss. 8. P. 1695–1702. 15. Teslina M. A., Ershova T. B., Vlasova N. M., Astapov I. A. Preparation of the MAX phase of the Ti-Al-C system by the powder metallurgy method. Perspektivnye materlialy. 2016. No. 3. pp. 75–80. 16. Song X.-J., Cui H.-Z., Hou N. et al. Lamellar structure and effect of Ti2AlC on properties of prepared in-situ TiAl matrix composites. Ceramics International. 2016. Vol. 42, Iss. 12. pp. 13586–13592. 17. Hu Ch., Zhou Y., Bao Y., Wan D. Tribological Properties of Polycrystalline Ti3SiC2 and Al2O3-Reinforced Ti3SiC2 Composites. Journal of the American Ceramic Society. 2006. Vol. 89, Iss. 1. pp. 3456–3461. |